- MJF gives a finer, more uniform surface and tighter batch-to-batch consistency.
- SLS has the larger build envelope and a lower setup, so one-offs are usually cheaper.
- Both are PA12 at roughly 175 °C HDT; neither is a high-temperature material.
- For 20+ identical parts, MJF is the default; for a 700 mm part, SLS is the only option.
The same polymer, two machines
SLS sinters powder with a laser, point by point. MJF deposits a fusing and a detailing agent across the whole bed, then applies infrared heat in one pass. The practical result is that MJF parts are denser and more uniform, with a finer grain and less variation between the top and bottom of the build.
Both processes are support-free. Both require escape holes for enclosed volumes. Both accept dye, paint and heat-set inserts. The differences are in surface, consistency and build size.
Surface and consistency
As printed, MJF reads as a fine matte grey; SLS reads as a slightly coarser, warmer grey. After dyeing, MJF holds a deeper, more even black because the surface is less porous.
Consistency matters more than either surface at volume. MJF holds dimensions across the build volume more tightly, which is why it is the usual choice for production-intent enclosures where part 200 must fit part 1.
Build size and design limits
SLS builds up to 700 × 380 × 380 mm; MJF tops out around 380 × 284 × 380 mm. That single number decides a lot of quotes: a 500 mm duct cannot be printed on MJF without splitting it.
Minimum wall is 0.8 mm on both, with 1.0 mm preferred for structural walls. MJF powder packs tighter, so use 4 mm escape holes rather than 3 mm where the geometry allows.
| Property | MJF | SLS |
|---|---|---|
| Build envelope | 380 × 284 × 380 mm | 700 × 380 × 380 mm |
| Typical surface | Fine, uniform matte | Coarser matte grain |
| Batch consistency | Very good | Good |
| Minimum wall | 0.8 mm | 0.8 mm |
| Escape holes | 4 mm recommended | 3 mm |
| Tolerance | ±0.3 mm or 0.3% | ±0.3 mm or 0.3% |
| Best at | 20–5,000 parts | 1–50 parts, large parts |
Cost: where the crossover is
MJF has a higher setup and a higher per-cm³ rate. At one part, SLS is usually cheaper. By 20–30 identical parts the consistency and surface of MJF usually justify the difference; by 100 parts the per-unit gap narrows to a few percent because both are dominated by material and machine time.
The quote tool applies the same volume discount to both, so you can switch the process and watch the delivered total change without re-uploading.
What we recommend
Prototype in SLS if the part is large, complex, or you need one quickly. Move to MJF when the design is stable and you need a batch that fits the same way every time.
If you need better heat or chemical resistance than PA12, neither process is the answer — look at PA12-GF, PA11 or a metal process instead.
Frequently asked
Is MJF more expensive than SLS?
Per cubic centimetre, yes, and the setup fee is higher. At low quantities SLS is cheaper. Above roughly 20–30 parts the difference per unit becomes small relative to the consistency gain.
Can MJF print PA11 or glass-filled nylon?
Our MJF line runs PA12. PA11 and PA12-GF are available on SLS, and both quote instantly in the same tool.
Which is better for living hinges?
Both work. MJF’s more uniform fusing gives slightly more predictable hinge fatigue, but hinge geometry and print orientation matter more than the machine.