- Keep beam strain under about 1% for resin, 4% for PA12, 2.5% for ABS/ASA.
- A longer beam is cheaper than a thicker one — length reduces strain quadratically.
- Print the beam in-plane so layers do not delaminate when it flexes.
- Always add a lead-in chamfer; a sharp undercut shaves material on the first assembly.
The geometry that matters
A cantilever snap is a beam of length L, thickness t and width b, with an undercut depth y. The strain at the root is approximately ε = 1.5 · t · y / L². Everything else — fillets, lead-in, retention angle — is secondary to those three numbers.
Because L is squared, doubling the beam length cuts strain by four. That is why the fix for a cracking snap is almost always “make the beam longer”, not “make it thicker”.
Allowable strain by material
Use these numbers for a single assembly; halve them for parts that will be opened repeatedly.
| Material | Allowable strain | Notes |
|---|---|---|
| Standard resin | 1.0% | Brittle; snap fits are a poor choice |
| Tough Resin | 2.0% | ABS-like, good for a few cycles |
| PA12 (SLS/MJF) | 4.0% | Best general choice for printed snaps |
| PA12-GF | 2.5% | Stiffer but more brittle than unfilled PA12 |
| TPU 95A | 8%+ | Flexible; use for seals and bumpers, not locating snaps |
| PLA (FDM) | 1.5% | Low; snaps crack along layer lines |
Worked example
A PA12 clip with a 1.2 mm thick beam, 0.4 mm undercut and 8 mm length: ε = 1.5 × 1.2 × 0.4 / 64 = 1.1%. That is well inside the 4% limit and will survive repeated opening.
Shorten the beam to 4 mm and the same geometry hits 4.5% — over the limit, and it will crack on the third or fourth cycle. Lengthen to 12 mm and it drops to 0.5%, which is conservative but may feel soft.
Orientation is half the design
FDM and resin parts are weakest between layers. If the beam bends across layer boundaries, it will delaminate at the root no matter how good the strain math is. Orient the print so the beam’s length lies in the build plane.
On SLS and MJF there are no layer boundaries in the same sense, but the beam still benefits from being in-plane because the powder bed gives slightly better resolution in X/Y than in Z.
Details that decide whether it clicks
These are the small features that separate a snap that works from one that shaves plastic on the first push.
- Lead-in chamfer: 30–45° over 0.5–1.0 mm, so the mating part cams the beam instead of cutting it.
- Retention face: 90° for permanent, 45–60° for releasable.
- Root fillet: 0.5 mm minimum; a sharp internal corner is a crack starter.
- Clearance behind the beam: at least the undercut depth plus 0.3 mm.
- Mating clearance: 0.2–0.3 mm per side on PA12; 0.15 mm on resin.
Frequently asked
Can I print a living hinge?
Yes, in PA12 or TPU. Use 0.35–0.5 mm thickness, a hinge length of at least 3× the thickness, and print it in-plane. Resin hinges work for a few cycles but fatigue quickly.
Why did my snap fit crack on the first assembly?
Usually one of: too-deep undercut, no lead-in chamfer, a sharp root, or layer lines across the bend. Send the model and we will flag the likely cause at review.
How much clearance should a snap need?
On PA12 allow 0.2–0.3 mm per side at the mating surfaces. On resin, 0.15 mm. Too little clearance turns a snap into an interference fit and the beam never deflects.