- Hole diameter for a heat-set insert is roughly the insert’s minor diameter minus 0.1–0.2 mm.
- Boss outside diameter should be at least 2× the insert diameter for PA12.
- Boss depth should exceed insert length by 0.5 mm so the insert seats below the rim.
- For resin, use a slightly larger boss and pre-heat the insert; resin splits more readily than nylon.
Three ways to put a thread in a printed part
Self-tapping screws are the cheapest option and the least durable: they cut their own thread once and strip if removed. Printed threads work for light duty and large sizes (M8+) but suffer from poor resolution at the crest. Heat-set inserts are the reliable option for anything that will be assembled more than twice.
The trade-off is space. An insert needs a boss, and a boss needs room that a thin wall does not have. Decide early, because retrofitting a boss often means reprinting the part.
| Method | Holds | Needs | Best for |
|---|---|---|---|
| Self-tapping screw | 1–3 cycles | Pilot hole, 0.8× screw dia | One-time assembly |
| Printed thread | 5–20 cycles | M8+, coarse pitch | Low-load, large threads |
| Heat-set insert | 50–100+ cycles | Boss + correct hole | Serviceable products |
| Through-bolt + nut | Unlimited | Access to both sides | Structural joints |
Sizing the hole and the boss
A heat-set insert is pressed in while hot, melting its way into the plastic. The hole should be slightly smaller than the insert’s outer diameter so material flows into the knurl: typically insert OD − 0.1 to − 0.2 mm on PA12, and OD − 0.05 mm on resin.
The boss outside diameter needs enough wall to resist hoop stress. For M3 inserts in PA12, a 6 mm boss is comfortable; 5 mm works but is tight. For resin, add 0.5 mm because it is more brittle.
| Insert | Hole (PA12) | Boss OD | Boss depth |
|---|---|---|---|
| M2.5 | 3.4 mm | 5.0 mm | 6.0 mm |
| M3 | 4.0 mm | 6.0 mm | 7.0 mm |
| M4 | 5.2 mm | 8.0 mm | 9.0 mm |
| M5 | 6.4 mm | 10.0 mm | 11.0 mm |
Installation without cracking the part
Set the soldering iron to roughly 250 °C for PA12 and 200 °C for resin, use a flat insert tip, and press straight down — not at an angle. Let the insert sink under light pressure; forcing it cold cracks the boss.
Support the boss from behind. A boss that hangs in free space will flex and split at the root. If the geometry allows, add a gusset or connect it to a nearby wall.
When not to use an insert
Very thin walls, small bosses under 4 mm, and parts that will be glued rather than serviced are all poor candidates. In those cases use a through-bolt with a nut, a threaded metal insert moulded into a larger assembly, or redesign the joint as a snap or a clamp.
If you are printing metal, printed threads are a different story — 316L and aluminium threads can be machined after printing to a real tolerance. Ask for CNC post-machining on the threaded features.
Frequently asked
What hole size for an M3 heat-set insert?
About 4.0 mm in PA12 and 4.1 mm in resin, assuming a standard 4.2–4.6 mm OD insert. Measure your insert; knurl depth varies by supplier.
Can I install inserts in SLS parts?
Yes, PA12 takes heat-set inserts very well. MJF is similar. Resin works but needs a gentler iron temperature and a thicker boss.
Do you install inserts?
We can supply and install inserts as a secondary operation on request; it is quoted separately from printing. Send the insert datasheet with the order.